Reading XANES Maps: Why a More Uniform Solid-State Cathode Can Have More Pores
A smooth voltage curve can average together particles that are deeply delithiated, particles that have barely started reacting, and particles that contribute little capacity. Synchrotron XANES imaging puts those differences back into space. A red–green map alone, however, does not tell us whether the cause is slow bulk diffusion, interfacial decomposition, or loss of contact.
Park and colleagues addressed this problem using single-crystal NCM622, Li₆PS₅Cl solid electrolyte, and a Li–In counter electrode. They compared bare cathode particles with particles coated in lithium difluorophosphate, LiDFP, combining in situ XRD, synchrotron TXM-XANES, and three-dimensional FIB-SEM statistics. Their most instructive finding is counterintuitive: the coated electrode reacted more uniformly and cycled better, yet had greater porosity and more geometrical contact loss. Pore volume alone therefore cannot explain its electrochemical degradation. Original paper
What was actually measured
The cathode was single-crystalline LiNi₀.₆Co₀.₂Mn₀.₂O₂, rather than polycrystalline secondary particles; the counter electrode was Li–In rather than lithium metal. The approximately 10 nm LiDFP layer was intended to suppress interfacial chemical degradation. Single crystals reduced the complication of intergranular cracking, making the interfacial comparison cleaner while limiting direct extrapolation to other particle architectures.
Blocking-electrode measurements supported the experimental design. Electronic conductivity decreased from 6.90×10⁻⁸ S/cm for the bare composite to 2.74×10⁻⁹ S/cm with coating, while ionic conductivities remained similar: 9.19×10⁻⁵ and 9.37×10⁻⁵ S/cm, respectively. Together with morphology and surface analysis, this supports a comparison centered on interfacial chemical reactivity. It does not establish that every interfacial property remained identical.
| Dataset | Conditions and method | What it establishes |
|---|---|---|
| Original Fig. 2a–d | Laboratory Cu Kα in situ XRD; 25 °C, 13 MPa; caption reports 0.48 mA/cm², text describes C/5 | Average lattice response and the distribution of diffraction peak positions |
| Original Fig. 2e–i | TXM-XANES at PLS-II beamline 7C, on cathode composites retrieved after electrochemical testing | Spatial chemical-state distributions at selected reaction states |
| Original Fig. 4a–f | FIB-SEM reconstruction after formation cycling; statistics on 500 labeled particles | Where pores and contact loss are distributed |
| Long-term cycling | 200 cycles at 13 MPa and C/4; a separate 500-cycle test at 120 MPa and C/2 | Durability under two distinct protocols |
The XANES measurements were ex situ, not a continuous operando movie of the same particles. The in situ diffraction was performed with a laboratory source. The paper gives 133 nm pixels in the results and an effective pixel size of approximately 135 nm in the methods, with a field of view around 273 μm. These describe approximately 0.13 μm sampling, not an independently demonstrated spatial resolution. Near the Ni K edge, images were collected at approximately 0.5–1 eV energy intervals, with 0.3 s exposure per image and subsequent alignment. Methods and full text
Original Figure 2: similar average curves conceal different particle populations

Figure 1. Reproduced unchanged from Park et al., Nature Communications 16, 8838 (2025), original Fig. 2. © The Author(s) 2025. DOI: 10.1038/s41467-025-63959-1, licensed under CC BY 4.0. Caption and interpretation added for this article.
Read panels a–d before e–i. Both electrodes delivered approximately 202 mAh/g on charge and had similar voltage trajectories in panel a. Yet the bare electrode developed pronounced splitting of the (003) reflection midway through charging, whereas the coated electrode showed more continuous solid-solution behavior. The split peaks indicate populations with different lattice states. They are not, by themselves, evidence for a newly discovered equilibrium phase diagram. The authors connect the apparent phase separation to particle-to-particle SOC differences and interfacial charge-transfer kinetics.
Panel d quantifies the distribution using a degree of heterogeneity, DOH. Its basis is the area-weighted variance of deconvoluted peak positions, multiplied by 10,000 for display. DOH is not a percentage of inactive particles, nor a universal number that can be compared across instruments without calibration. The bare sample exceeded 50 at SOC 40, SOC 80, and the end of the first discharge; the coated sample stayed below 40 across the reported SOC range. Comparisons require consistent peak fitting, resolution, and background treatment. Strain, broadening, and fitting choices can also affect the metric.
Panels e and f supply spatial chemical evidence. An energy scan yields a Ni K-edge XANES spectrum at each valid pixel. The authors used the spectral peak energy as a descriptor of Ni chemical state, with an SOC reference measured in liquid-electrolyte NCM. These colors do not directly image lithium atoms or provide an error-free lithium concentration at every pixel. They first represent a Ni chemical-state distribution, which is interpreted in terms of reaction progress using calibration and electrochemistry.
The numbers matter more than the palette. At SOC 40, the standard deviation of peak energy was 0.689 eV for bare NCM and 0.387 eV for coated NCM. At SOC 80 it was 0.552 versus 0.246 eV; at the end of discharge, 0.500 versus 0.329 eV. Calculated from the figure, the width decreased by approximately 44% and 55% at the two charging states. Those percentages describe spectral-energy standard deviations, not a directly measured percentage reduction in lithium-concentration heterogeneity. The discharge endpoints also differed: residual SOC was 24.9 for bare NCM and 20.1 for the coated sample, so that pair is not a strictly matched-SOC comparison.
The histograms in g–i distinguish movement of the mean from narrowing of the distribution. Bare NCM exhibits split or two-population distributions at SOC 40 and 80, while the coated sample is more concentrated. This agrees with the XRD peak splitting and DOH trends. Two different physical observables support heterogeneous particle participation, rather than the interpretation resting on a colored image alone. Figure 2 and results
A useful additional control was aging: a bare electrode left assembled for 72 h without operation subsequently showed stronger (003) splitting. This supports the idea that chemical degradation upon contact can amplify heterogeneity even before high-current cycling. XANES did not directly measure a local interface resistance, however. The proposed chain—interphase growth, slower charge transfer, and divergent particle SOC—depends on the combined TOF-SIMS, impedance, and diffraction evidence.
Original Figure 4: more pores do not necessarily mean worse cycling

Figure 2. Reproduced unchanged from the same paper, original Fig. 4. © The Author(s) 2025, CC BY 4.0. Source: Park et al., 2025.
Panels a–c compare the surface area, volume, and surface-to-volume ratio of 500 labeled particles. Similar distributions help rule out a gross particle-size difference as the explanation for subsequent comparisons. The reconstructed volume was approximately 28.28×39.08×55.82 μm³. It contains much more complete adjacency information than a two-dimensional section, but remains a finite, destructively sampled volume.
Panel d reports porosities of 5.54% for bare NCM and 7.16% for coated NCM, with ionic tortuosities of 1.33 and 1.48. In panel e, the slope of contact-loss area versus particle surface area increases from 0.132 to 0.255, corresponding to approximately 13.2% and 25.5% geometrical contact loss. A simple rule that more pores, more tortuous paths, and less direct contact must imply poorer cycling would therefore predict the wrong outcome.
Panel f provides the missing spatial context. At equal contact-loss area, the fitted adjacent-pore-volume slopes are 4.650 for bare NCM and 3.366 for coated NCM—a ratio around 1.38 from the displayed values, reported as about 1.39 in the paper's text. Bare NCM develops fewer, larger, concentrated pores; coated NCM develops more numerous, smaller, more uniformly distributed pores. This is consistent with the reaction maps: broader particle participation can produce widespread small gaps, whereas uneven reaction can concentrate morphological change. It does not mean that pores improve cycling.
The GITT analysis in g and h separates geometrical contact from effective electrochemical area. The protocol used 10 min discharge steps followed by 50 min relaxation. The interpretation relies on the relation between (ΔEₛ/ΔEₜ)² and D×S². If bulk diffusivity is comparable between samples at the same SOC, a larger response can indicate a larger effective active area. The authors propose that a coating remaining in contact with NCM can supply lateral ion-conduction pathways, allowing some surface that lacks direct contact with sulfide electrolyte to remain electrochemically accessible.
This is a supported mechanism, not a direct movie of interfacial ion transport or an independent measurement of absolute diffusivity. GITT interpretation depends on assumptions about diffusion, contact area, and equilibration; several impedance contributions can influence the voltage response. The defensible conclusion is that geometrically separated surface and electrochemically inactive surface need not coincide. Figure 4 and GITT discussion
Performance numbers must retain their conditions. At 13 MPa and C/4, capacity retention after 200 cycles was 84% for coated NCM and 26.9% for bare NCM. In a separate 120 MPa, C/2 test, retention after 500 cycles was 87.5% and 59.9%. The latter is high-pressure evidence, not low-pressure engineering validation. Figure 4i compares 2.6, 3.3, and 6.5 MPa at 25 °C and C/10, with 7.4 mg/cm² active-material loading. Stable operation of coated NCM for more than ten cycles at 3.3 MPa is a useful control, but its observation window is too short to replace a long-term lifetime test.
Designing the next XANES experiment
The practical lesson is to treat a reaction distribution as a quantity requiring validation. At matched SOC, report the mean, distribution width, and population structure. Check whether another structural observable supports the same heterogeneity, then connect the result to interface chemistry, contact geometry, and electrochemical performance under consistent conditions.
Keep the raw energy scans, calibration and drift records, dark- and flat-field corrections, pixel masks, alignment parameters, and fit residuals. Report both pixel distributions and particle-averaged distributions: pixels are not independent replicates, and larger particles contribute more pixels. A claim of dynamic propagation requires sufficiently fast operando measurements, explicit timestamps, and beam-dose controls. The selected-SOC ex situ maps here support comparisons between states; they do not record the continuous trajectory of the same particle. Respecting that distinction is what turns an attractive image into credible mechanistic evidence.
Reference: Park, C., Choi, J., Park, S. et al. Interfacial chemistry-driven reaction dynamics and resultant microstructural evolution in lithium-based all-solid-state batteries. Nature Communications 16, 8838 (2025). DOI · Open full text and supplementary-material links. This is an independent commentary; the original authors do not endorse this blog.