Not every crack is equally dangerous: mapping solid-state battery failure with synchrotron tomography
A crack in a tomographic image is only the beginning of an explanation for a solid-state battery short circuit. Does it span the electrolyte thickness? Has nearby material reacted? Is the local region under tension or compression? Was the defect created during cycling, or inherited from processing and assembly? A grayscale slice alone cannot usually resolve these questions.
The study by Hu and colleagues in Advanced Energy Materials combines X-ray micro-computed tomography, μ-CT, with diffraction computed tomography, XRD-CT. Imaging reveals morphology; diffraction identifies crystalline phases and provides lattice parameters from which elastic strain can be estimated. Published online in December 2024 and assigned to a 2025 journal issue, the work compares pristine and failed cells in three-dimensional in situ measurements. It is not a continuous operando movie of an entire cycle history. That distinction matters when interpreting causality.
Figure 1: through-thickness cracks identify candidates, not the proven current path

Original Figure 1, reproduced in full. a: pristine Li₆PS₅Cl pellet and a near-interface section. b: cell cycled to short circuit. c: perpendicular sections through b, with through-thickness “terminal cracks” highlighted in magenta. The symmetric cell was cycled at room temperature, without additional stack pressure, at 0.3 mA cm⁻² and shorted after approximately 12 h. Source: Hu et al., Advanced Energy Materials 15, 2404231 (2025; first published online in 2024), DOI. © 2024 The Author(s), CC BY 4.0. Extracted from the published PDF; data and labels are unchanged.
The cells are symmetric Li|Li₆PS₅Cl|Li devices; Li₆PS₅Cl is abbreviated LPSC here. The pristine pellet in Figure 1a is relatively uniform, apart from a few isolated defects. The failed cell in b contains numerous cracks extending inward from the lithium/electrolyte interfaces. Panel c adds a crucial dimension: a long crack in a horizontal slice need not traverse the pellet thickness. Three-dimensional connectivity identifies paths that could connect the opposing electrodes.
The authors call cracks spanning the entire electrolyte thickness “terminal cracks.” This is a geometric classification. It does not demonstrate that each crack is filled with metallic lithium, or directly identify which one conducted first. The paper explicitly leaves the precise short-circuit path unresolved and treats the through-thickness cracks as candidates. Describing the magenta lines as directly imaged lithium dendrites would exceed the evidence.
Resolution also constrains the interpretation. The shorted-cell μ-CT voxel size is approximately 0.70 μm, but the authors consider only cracks above roughly 5 μm reliably segmentable. Voxel size is not the minimum reliably detected crack width. Finer cracks, nanoscale voids and narrow lithium pathways may still matter electrochemically. The pristine-cell effective pixel size is approximately 0.65 μm, and the two imaging datasets used different beamline/energy conditions. Their pronounced large-scale morphological contrast is compelling; subtle grayscale differences should not be turned into precise density changes.
The approximately 12 h failure time applies to this room-temperature symmetric-cell experiment at 0.3 mA cm⁻², without additional stack pressure. It is not an intrinsic LPSC lifetime, nor a prediction for full cells with different pressure, sealing or interface treatments. Symmetric cells isolate lithium/electrolyte behavior but omit the additional reactions and constraints of a composite positive electrode.
Figure 2: similar grayscale can conceal different chemistry

Original Figure 2, reproduced in full. A shorted-cell section 120 μm from the Li|LPSC interface, with corresponding μ-CT and crystalline-phase maps. The LPSC colorbar is integrated (111) diffraction intensity in arbitrary units; the other phase colorbars report volume percentages. These scales must not be conflated. Source: Hu et al., DOI. © 2024 The Author(s), CC BY 4.0. Reproduced without modification.
Start with the purple ellipse near the upper-right edge of the LPSC map. Its LPSC diffraction signal is lower, yet the matching μ-CT region is not an obvious void. The Li₂CO₃ and LiCl maps show enrichment at the same location, with Li₂S also present. The authors interpret this as a pocket of incompletely mixed or reacted precursor material affected by air-related chemistry. The low-LPSC region still contains approximately 80% LPSC; it is not a completely decomposed volume.
This is the benefit of combining modalities. Imaging contrasts related to attenuation and phase can have difficulty separating materials of similar density. XRD-CT adds crystalline identity. However, the heat maps cannot be compared by color alone. LPSC is shown through its integrated (111) peak intensity in arbitrary units, whereas the secondary-phase maps show refined volume fractions. Calling all bright areas the same percentage would invent a quantitative relationship that the figure does not provide.
Nor should every secondary phase be attributed to cycling. Li₂S and LiCl are also LPSC synthesis precursors: they may remain from processing or occur in decomposition chemistry. Carbon and Li₂C₂ are associated with the heat-treatment history, while Li₂CO₃ indicates involvement of air/CO₂. Li₃P was detected below 0.5 vol% and was not discussed in detail further. The valuable result is not simply a longer list of detected compounds, but the use of spatial co-location and preparation history to constrain their origins.
The large crack within the green ellipse lacks the carbonate enrichment seen at some other cracks. The authors propose that earlier, accessible cracks had opportunities to react with residual air, whereas a later crack filled with lithium might not. This is a plausible explanation, not a directly recorded chronology. Absence of carbonate alone cannot establish that a crack has just formed; signal strength, detection limits and gas accessibility also matter.
Metallic lithium itself is another limitation. Its weak scattering and locally inadequate powder averaging made a reliable diffraction reconstruction difficult. Near-interface lithium fractions were obtained in part through segmentation of corresponding μ-CT data. These maps therefore connect morphology, reaction phases and lattice changes; they are not a direct, quantitative metallic-lithium concentration map at every pixel.
Figure 3: quantify the interface-to-bulk contrast

Original Figure 3, reproduced in full. a: void/crack fraction through the electrolyte thickness. b: phase fractions near the shorted-cell interface. c: LPSC fractions in the two cells. d: mean volumetric elastic strain derived from LPSC lattice parameters and the corresponding stress conversion. Relevant error bars describe spatial dispersion among voxels at a given depth, not confidence intervals from many independent cell-lifetime tests. Source: Hu et al., DOI. © 2024 The Author(s), CC BY 4.0. Reproduced without modification.
Figure 3a turns the visual contrast into a depth profile. The shorted cell reaches near-interface defect fractions above 20%, compared with approximately 1–2% in the bulk. This localizes degradation near the lithium contacts. It does not mean that one-fifth of the whole electrolyte pellet has disappeared: the values belong to sections at particular depths, not to the entire cell volume.
Panels b and c show reduced LPSC and increased secondary phases within approximately 20 μm of the interface, notably Li₂CO₃. An especially revealing baseline is the pristine cell: it already contains only about 85% LPSC, with approximately 15% secondary phases before cycling. These are values for this sample and refinement framework, not a general purity specification for LPSC. They show why cycling-induced changes must be interpreted against a measured processing and assembly baseline.
Panel d links the chemical and mechanical pictures. At each voxel, the LPSC lattice parameter a is compared with a reference a₀ to obtain volumetric strain, εᵥ = (a³ − a₀³)/a₀³. The authors convert this to equivalent volumetric stress using K = 18.4 GPa. Positive values denote tension and negative values compression. The shorted cell reaches a mean tensile stress of approximately 30 MPa near the interface, while the pristine cell remains close to zero across the measured depths.
The 30 MPa value is not a directly measured contact pressure, nor a full three-dimensional stress tensor. The calculation treats the bulk region more than roughly 15 μm from the interface as an overall stress-free reference and represents the actual anisotropic field by an equivalent isotropic volumetric quantity. Lattice parameters measure elastic strain; they do not automatically include plastic deformation. Meaningful comparisons must therefore specify the reference lattice, modulus and strain definition. Identically labeled MPa values can otherwise refer to different physical quantities.
The paper compares approximately 30 MPa with an order-of-magnitude yield stress of 1 MPa for macroscopic metallic lithium, suggesting mechanical conditions capable of pushing lithium into cracks. This is a useful scale comparison, not a universal threshold for nanoconfined lithium. Yield behavior depends on size, temperature and strain rate. Similarly, larger error bars principally indicate stronger spatial heterogeneity; they do not mean the mean is necessarily erroneous or that many independent cells have established the same lifetime prediction.
What does the combined map change about the experiment?
The synchrotron contribution is more than a sharper image. High-energy, high-flux measurements at ESRF allow weak secondary-phase diffraction signals to be registered with detailed morphology. For the shorted cell, XRD-CT used a 72.5 keV beam focused to approximately 10 × 5 μm, with matching raster steps. The μ-CT voxel size was much smaller, around 0.70 μm. Registration does not remove that resolution difference: diffraction near a narrow crack can average several phases and local environments. Each fine CT voxel does not have its own independent stress measurement at the same resolution.
Together, the three figures shift the objective from removing every visible crack toward identifying connected defects associated with high tensile stress or chemical hotspots. They also make precursor mixing, heat treatment, sealing and cycling separate experimental variables. Increasing stack pressure cannot be declared a universal remedy from this work: mechanical constraints affect both crack propagation and lithium flow, and the study did not perform a systematic pressure sweep.
The most persuasive next step is time-resolved multimodal tracking of selected high-risk regions in the same cell, with verified sealing, appropriate replication and controlled beam effects. That could test whether reaction products precede stress concentration, and when a connected crack becomes occupied by lithium. This paper provides a three-dimensional basis for choosing what to follow. It does not yet turn endpoint correlations into a complete temporal sequence of failure.
Verification links: original article and supporting information; published PDF in the Oxford open repository. This is a literature analysis. Reproduced measurements and numerical results belong to the cited authors; proposed explanations are distinguished from direct observations.